Researchers have examined whether four commercial natural colorants can be compounded into biodegradable polyesters on standard melt-processing equipment. The results show that most pigment–polymer combinations survive extrusion with only modest changes to flow and mechanical behavior, while long-term color stability remains the main obstacle.
The study, titled “Sustainability in the Development of Natural Pigment-Based Colour Masterbatches and Their Application in Biopolymers,” used blue spirulina, yellow curcumin, red beetroot and green chlorophyllin. Each pigment was combined with polylactic acid (PLA) and polybutylene succinate (PBS) to produce color masterbatches on a twin-screw extruder. The formulations also contained titanium dioxide, calcium carbonate and stearic acid to support UV protection, dispersion and processing. The masterbatches were then let down into the matching polymer at 2, 4 and 6 wt% and injection molded into test specimens.
Thermal window sets the limits
Because natural colorants are organic, they can begin to degrade at temperatures below those needed to melt the carrier polymer. Thermogravimetric analysis put degradation onset at roughly 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot, all well under the degradation temperatures of PLA and PBS themselves. The researchers therefore chose extrusion profiles that melted each polymer while limiting heat exposure to the pigment: about 145 °C for PBS and 190 °C for PLA, with the twin-screw running at 65 rpm and a feed rate of 2 kg/h.
That window suited most pigment–polymer pairs, but spirulina was the exception. Processed in PLA at 190 °C, it lost its characteristic blue color, so a blue PLA masterbatch could not be produced. In PBS, whose lower processing temperature was gentler on the pigment, compounding succeeded. The study concludes that pigment compatibility is closely tied to the thermal requirements of the matrix, not to the colorant alone.
Flow and mechanical properties largely preserved
Rheology changed little. Melt flow rate fell only slightly after pigment addition, pointing to a modest rise in melt viscosity. Neat PLA measured around 50 g/10 min, and the natural-pigment masterbatches stayed near that figure; PBS responded in similar fashion. For compounders this matters, because a color system that forces redesign of screws, pressure settings or molding conditions has little practical value. Here, conventional twin-screw compounding and injection molding handled most formulations without major processing problems.
Tensile and impact behavior also held. PLA began at a Young’s modulus of about 1710 MPa and a tensile strength of 65.6 MPa, while PBS started near 392 MPa and 34.5 MPa. Across the 2–6 wt% range the colored formulations stayed close to those baselines, and impact strength remained in a similar band, although individual pigments produced some variation.
Light stability is the largest barrier
Successful extrusion did not translate into durable color. After 50 hours of xenon-lamp exposure, most formulations exceeded a color difference of ΔE* = 2, a level the researchers associate with a visually perceptible change. The PLA compound containing 2 wt% green chlorophyllin masterbatch was the main exception and showed the highest photostability.
The study identifies UV stability as the biggest obstacle to wider adoption. Packaging, consumer products, agricultural parts and outdoor applications would likely need additional stabilization, protective coatings or pigment modification before natural colors could match conventional systems over long service periods.
Lower carbon footprint
The environmental comparison favored the bio-based colorants. Under the study’s assumptions, one kilogram of curcumin pigment was associated with about 0.04 kg CO2-eq, against 18.65 kg CO2-eq for the inorganic green reference pigment. The natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing.
The researchers note that natural pigment masterbatches still require further development, especially in lightfastness and thermal stability. Even so, the trial shows that several natural colorants can be compounded into PLA and PBS on conventional equipment with limited penalty in melt viscosity or mechanical performance, and the authors argue that future work should focus on color retention during processing and subsequent service exposure.